STYROFOAM™ HD300
| Properties |
Standard |
Unit |
STYROFOAM HD300 |
| Density, min. |
DIN 53420
ASTM D 1622 |
kg/m3
lb/ft3 |
45
2,8 |
Thermal conductivity at 10 °C (50°F)
mean temperature of test
mean temperature 23,9° C (75°F) |
DIN 52612
DIN 52616
ASTM C 177-97 or
ASTM C 518-98 |
W/m . K
Btu . In/ft2 . H . °F |
0,026
0,18 |
| Compressive strength at 10% deflection |
DIN 53421
ASTM D 1621-95 |
kPa
psi |
700
100 |
| Water absorption by submersion |
DIN 53428
ASTM D 2842 (±1% by vol.precision) |
% by Vol.
% by Vol. |
0,2
> ≤ 1 |
Water vapour diffusion resistance factor µ
Water vapour permeability 1) |
DIN 52615
ASTM E 96-00 |
--
Perm-inch |
150-220
0,4 |
| Capillarity |
-- |
-- |
none |
| Heat stability / compressive creep |
DIN 18164 |
20 kPa, 80°C
Type 2,8 psi,
176°F
40 kPa, 70°C
Type 5,6 psi,
158°F |
WD
WS |
| Linear coefficient of thermal expansion and contraction (heating soaking conditions) |
DIN 52328 |
°C-1
°F-1 |
70.10-6
39.10-6 |
| Irreversible dimensional variation (result of laboratory test with temperature changes up to 60° C (104°F) |
-- |
% |
< 0,2 |
| Fire classification (Germany) |
DIN 4102 |
Building material class |
B2 |
| Underwriters Laboratories (UL) classification according to ASTM-E-84 Standard Test Method for Surface Burning Characteristics of Building Materials under designation ASTM C 578-95 2) |
Flame spread
Smoke developed
for max 4 pcf
density and 4” max
thickness |
-- |
5
165 |
Dimensions (mm)
Width
Length
Thickness |
-- |
-- |
600
1250
20-100 |
Appearance
Surface
Edge profile |
-- |
-- |
skin
shiplap
 |
1) value is thickness related
2) upon special request charging additional cost
|
|